UV Curing: Difference between revisions

From ProtoFab
Jump to navigation Jump to search
Content deleted Content added
Added how to read UV intensities pictures/graphs
No edit summary
Line 1: Line 1:
Supplier's Recommended UV Intensity can be used as baseline. If another intensity is needed, us the following graphs to determine irradiation area and working distance.
Supplier's Recommended UV Intensity can be used as baseline. If another intensity is needed, us the following graphs to determine irradiation area and working distance.

[[File:How to read UV intensity1.png|left|thumb|744x744px|How to read UV intensities]]
[[File:ANUJ6170 UV Intensity Profile.png|none|thumb|595x595px|UV Intensities using ANUJ6170 head and ANUJ6428 lens]]


== UV Curing Recipes ==
== UV Curing Recipes ==

Revision as of 11:09, 31 August 2026

Supplier's Recommended UV Intensity can be used as baseline. If another intensity is needed, us the following graphs to determine irradiation area and working distance.


UV Curing Recipes

Recipes for hybrid materials are for initial tack only. UV exposure and heat cure will typically be needed for 100% crosslink.

UV Curing
Material Supplier's Recommended

UV Intensity

Controller Output Time LED Distance From Sample Additional Heat Cure(Temp°C/Time)
OG116-31 100% 330 sec 1cm
HYB-353ND 100mW/cm2 100% 60 sec 1cm 100°C / 30 min
3553-LV-UTF_HM 1000mW/cm2 100% 30 sec 1cm 120°C/30 min